At a glance
Based on the row for liquid, 20 °C.
- Rated A, very good resistance
- PTFE, PVDF, PVC Rigid, Viton (FPM), NBR, SS 316, SS 304, Aluminium, FEP, Nylon (PA), Acetal (POM), PETG, SAN (13)
- Rated B, good resistance
- LDPE (1)
- Rated C, limited resistance
- PP, Polycarbonate (2)
- Rated D, not resistant
- EPDM, Polystyrene, PMP (3)
- No data in the source
- HDPE, ECTFE/ETFE, Silicone, PVC Flexible, Polysulfone
- Rated lower at 50 °C than at 20 °C
- PP (C → D), PVC Rigid (A → C), LDPE (B → C), SAN (A → C)
Based on the row for liquid, 20 °C.
Rating profile by material family
Effect of temperature, 20 °C to 50 °C
Substance
- Hazard symbols in the source
- Xn (harmful), N (dangerous for the environment) (pre-GHS European symbols; check the current safety data sheet)
- Flammable
- yes
- Concentrations listed
- liquid
- Name in the source (German)
- Testbenzin
Resistance table: White Spirit, liquid
| Material | 20 °C | 50 °C | Remark |
|---|---|---|---|
| Thermoplastics | |||
| LDPE | B | C | |
| PP | C | D | |
| PVC Rigid | A | C | |
| PMP | D* | – | |
| Polystyrene | D | D | |
| SAN | A | C | |
| Polycarbonate | C* | – | |
| PETG | A | – | |
| Acetal (POM) | A | – | |
| Nylon (PA) | A* | – | |
| Fluoropolymers | |||
| PTFE | A | A | |
| FEP | A* | – | |
| PVDF | A* | – | |
| Elastomers | |||
| EPDM | D | D | |
| Viton (FPM) | A | A | |
| NBR | A | – | |
| Metals | |||
| SS 316 | A | A | |
| SS 304 | A | A | |
| Aluminium | A | A | |
* estimated rating, given in the source without a temperature
Not rated in the source, so not in the table: HDPE, PVC Flexible, Polysulfone, ECTFE/ETFE, Silicone
Rating scale
- A very good resistance
- B good resistance
- C limited resistance
- D not resistant
- – no data
- K no general statement possible
A rating marked * is an estimate in the source, not a test result. An estimate is given as one value without a temperature.
About this data
The ratings come from the chemical resistance list published by Bürkle GmbH, which compiled them from raw-material manufacturers’ data. They describe laboratory tests on the raw material at 20 °C and 50 °C.
A finished part also sees pressure, mechanical stress, welds and mixtures that a laboratory test does not. Treat the rating as a first filter and test under your own conditions before relying on it.
Chemicals with a similar resistance profile
Same 20 °C rating on the share of materials shown.