Summary
- Silicone is rated better with
- Salts and salt solutions (+12 points)
Points are the difference in the share of rows rated A or B.
The two materials
Viton (FPM)
Fluoroelastomer (FKM/FPM)
Fluoroelastomer (Viton, FKM/FPM) resists fuels, oils and many acids. Ketones, esters, amines and hot water or steam attack it.
Rated rows: 965. A 57 %, B 10 %, C 18 %, D 15 %
Silicone
Silicone rubber
Silicone rubber keeps its flexibility over a wide temperature range. Concentrated acids and alkalis and hydrocarbon solvents attack or swell it.
Rated rows: 23. A 96 %, B 0 %, C 0 %, D 4 %
Share of rows rated A or B, by chemical class
How often the two ratings agree
Chemical classes were assigned by this site, not by the source. Mixtures and trade products without a clear class are not counted.
By chemical class
| Chemical class | Viton (FPM): rated A or B | Silicone: rated A or B |
|---|---|---|
| Mineral acids | 83 % (63 rows) | – |
| Organic acids | 62 % (64 rows) | – |
| Alkalis | 55 % (22 rows) | – |
| Salts and salt solutions | 88 % (198 rows) | 100 % (9 rows) |
| Oxidising agents and halogens | 77 % (62 rows) | – |
| Alcohols and glycols | 69 % (58 rows) | – |
| Phenols | 29 % (14 rows) | – |
| Ketones and aldehydes | 6 % (35 rows) | – |
| Esters and ethers | 15 % (71 rows) | – |
| Amines and nitrogen compounds | 24 % (37 rows) | – |
| Aromatic hydrocarbons | 64 % (14 rows) | – |
| Fuels, mineral oils and aliphatic hydrocarbons | 90 % (71 rows) | – |
| Vegetable and animal oils, fats, essential oils | 83 % (48 rows) | – |
| Halogenated hydrocarbons | 33 % (70 rows) | – |
| Foods and beverages | 96 % (46 rows) | – |
Where the ratings differ most
Rows where the two ratings at 20 °C are at least two grades apart: 1 in total.
| Chemical | Concentration | Viton (FPM) | Silicone |
|---|---|---|---|
| Chromic-Sulfuric Acid | concentrated | A | D |
Rating scale
- A very good resistance
- B good resistance
- C limited resistance
- D not resistant
- – no data
- K no general statement possible
A rating marked * is an estimate in the source, not a test result. An estimate is given as one value without a temperature.
More comparisons
Frequently Asked Questions
Is Viton (FPM) or Silicone more chemical-resistant?
Of 22 chemicals rated for both materials at 20 °C, Viton (FPM) and Silicone share the same rating in 21 rows (95 %). Viton (FPM) is rated better in 1 rows and Silicone in 0 rows.
How do Viton (FPM) and Silicone compare for chemical resistance?
Based on 22 chemicals tested for both: Viton (FPM) is rated better with –. Silicone is rated better with Salts and salt solutions. They perform similarly with –.
About this data
The ratings come from the chemical resistance list published by Bürkle GmbH, which compiled them from raw-material manufacturers’ data. They describe laboratory tests on the raw material at 20 °C and 50 °C.
A finished part also sees pressure, mechanical stress, welds and mixtures that a laboratory test does not. Treat the rating as a first filter and test under your own conditions before relying on it.