ChemicalResistance
ChemicalResistance.org

Sodium Nitrate Chemical Resistance

Resistance ratings for 24 plastics, elastomers and metals at 20 °C and 50 °C. Listed at 2 concentrations, because the rating depends on it.

At a glance

Based on the row for saturated, 20 °C.

Rated A, very good resistance
PTFE, HDPE, PP, PVDF, PVC Rigid, EPDM, Viton (FPM), SS 316, SS 304, Aluminium, LDPE, FEP, ECTFE/ETFE, Nylon (PA), Acetal (POM), Polycarbonate, PVC Flexible, Polystyrene, Polysulfone, PETG, PMP, SAN (22)
Rated B, good resistance
NBR (1)
Rated C, limited resistance
none (0)
Rated D, not resistant
none (0)
No data in the source
Silicone
Rated lower at 50 °C than at 20 °C
PVC Rigid (A → C), NBR (B → C), PVC Flexible (A → C)
Rating changes with concentration (20 °C)
NBR: A (aqueous), B (saturated)

Based on the row for saturated, 20 °C.

Rating profile by material family

Sodium Nitrate: Rating profile by material familyThermoplastics: 13 A. Fluoropolymers: 4 A. Elastomers: 2 A, 1 B, 1 no data. Metals: 3 A.Thermoplastics (13)Thermoplastics: 13 × A, very good resistance (HDPE, LDPE, PP, PVC Rigid, PVC Flexible, PMP, Polystyrene, SAN, Polycarbonate, PETG, Acetal (POM), Nylon (PA), Polysulfone)A 13Fluoropolymers (4)Fluoropolymers: 4 × A, very good resistance (PTFE, FEP, PVDF, ECTFE/ETFE)A 4Elastomers (4)Elastomers: 2 × A, very good resistance (EPDM, Viton (FPM))A 2Elastomers: 1 × B, good resistance (NBR)B 1Elastomers: 1 × no data (Silicone)– 1Metals (3)Metals: 3 × A, very good resistance (SS 316, SS 304, Aluminium)A 3
A very good resistanceB good resistanceC limited resistanceD not resistantno data
Number of materials in each family with each rating at 20 °C.

Effect of temperature, 20 °C to 50 °C

Sodium Nitrate: Effect of temperature, 20 °C to 50 °CPVC Rigid A → C; PVC Flexible A → C; NBR B → C.ABCDPVC Rigid: A at 20 °C, C at 50 °CPVC RigidPVC Flexible: A at 20 °C, C at 50 °CPVC FlexibleNBR: B at 20 °C, C at 50 °CNBR
20 °C50 °C
Materials whose rating differs between 20 °C and 50 °C. Materials not shown keep their rating or have no 50 °C value.

Substance

CAS number
7631-99-4
Formula
NaNO3
Hazard symbols in the source
O (oxidising), Xn (harmful) (pre-GHS European symbols; check the current safety data sheet)
Concentrations listed
aqueous; saturated
Name in the source (German)
Natriumnitrat

Rating by concentration

Sodium Nitrate: Rating by concentrationHDPE: aqueous A, saturated A. LDPE: aqueous A, saturated A. PP: aqueous A, saturated A. PVC Rigid: aqueous –, saturated A→C. PVC Flexible: aqueous –, saturated A→C. PMP: aqueous –, saturated A. Polystyrene: aqueous –, saturated A. SAN: aqueous –, saturated A. Polycarbonate: aqueous A, saturated A. PETG: aqueous A, saturated A*. Acetal (POM): aqueous A, saturated A. Nylon (PA): aqueous A, saturated A. Polysulfone: aqueous –, saturated A. PTFE: aqueous A, saturated A. FEP: aqueous A, saturated A. PVDF: aqueous A, saturated A. ECTFE/ETFE: aqueous A, saturated A. EPDM: aqueous A, saturated A. Viton (FPM): aqueous A, saturated A. NBR: aqueous A, saturated B→C. SS 316: aqueous A, saturated A. SS 304: aqueous A, saturated A. Aluminium: aqueous A, saturated A.aqueoussaturatedTHERMOPLASTICSHDPEHDPE, aqueous: A at 20 °C, A at 50 °CAHDPE, saturated: A at 20 °C, A at 50 °CALDPELDPE, aqueous: A at 20 °C, A at 50 °CALDPE, saturated: A at 20 °C, A at 50 °CAPPPP, aqueous: A at 20 °C, A at 50 °CAPP, saturated: A at 20 °C, A at 50 °CAPVC RigidPVC Rigid, aqueous: no data–PVC Rigid, saturated: A at 20 °C, C at 50 °CA→CPVC FlexiblePVC Flexible, aqueous: no data–PVC Flexible, saturated: A at 20 °C, C at 50 °CA→CPMPPMP, aqueous: no data–PMP, saturated: A at 20 °CAPolystyrenePolystyrene, aqueous: no data–Polystyrene, saturated: A at 20 °C, A at 50 °CASANSAN, aqueous: no data–SAN, saturated: A at 20 °C, A at 50 °CAPolycarbonatePolycarbonate, aqueous: A at 20 °CAPolycarbonate, saturated: A at 20 °CAPETGPETG, aqueous: A at 20 °CAPETG, saturated: A at 20 °C (estimate)A*Acetal (POM)Acetal (POM), aqueous: A at 20 °C, A at 50 °CAAcetal (POM), saturated: A at 20 °C, A at 50 °CANylon (PA)Nylon (PA), aqueous: A at 20 °CANylon (PA), saturated: A at 20 °CAPolysulfonePolysulfone, aqueous: no data–Polysulfone, saturated: A at 20 °CAFLUOROPOLYMERSPTFEPTFE, aqueous: A at 20 °C, A at 50 °CAPTFE, saturated: A at 20 °C, A at 50 °CAFEPFEP, aqueous: A at 20 °C, A at 50 °CAFEP, saturated: A at 20 °C, A at 50 °CAPVDFPVDF, aqueous: A at 20 °C, A at 50 °CAPVDF, saturated: A at 20 °C, A at 50 °CAECTFE/ETFEECTFE/ETFE, aqueous: A at 20 °C, A at 50 °CAECTFE/ETFE, saturated: A at 20 °C, A at 50 °CAELASTOMERSEPDMEPDM, aqueous: A at 20 °CAEPDM, saturated: A at 20 °CAViton (FPM)Viton (FPM), aqueous: A at 20 °C, A at 50 °CAViton (FPM), saturated: A at 20 °C, A at 50 °CANBRNBR, aqueous: A at 20 °CANBR, saturated: B at 20 °C, C at 50 °CB→CMETALSSS 316SS 316, aqueous: A at 20 °C, A at 50 °CASS 316, saturated: A at 20 °C, A at 50 °CASS 304SS 304, aqueous: A at 20 °C, A at 50 °CASS 304, saturated: A at 20 °C, A at 50 °CAAluminiumAluminium, aqueous: A at 20 °C, A at 50 °CAAluminium, saturated: A at 20 °C, A at 50 °CA
A very good resistanceB good resistanceC limited resistanceD not resistantno data
Each cell shows the rating at 20 °C. Where the rating at 50 °C differs, it follows the arrow. * marks an estimate in the source.
Show as a table
Materialaqueoussaturated
Thermoplastics
HDPEAA
LDPEAA
PPAA
PVC Rigid–A
PVC Flexible–A
PMP–A
Polystyrene–A
SAN–A
PolycarbonateAA
PETGAA*
Acetal (POM)AA
Nylon (PA)AA
Polysulfone–A
Fluoropolymers
PTFEAA
FEPAA
PVDFAA
ECTFE/ETFEAA
Elastomers
EPDMAA
Viton (FPM)AA
NBRAB
Silicone––
Metals
SS 316AA
SS 304AA
AluminiumAA

* estimated rating, given in the source without a temperature

Resistance table: Sodium Nitrate, aqueous

Material20 °C50 °CRemark
Thermoplastics
HDPEAA
LDPEAA
PPAA
PolycarbonateA–
PETGA–
Acetal (POM)AA
Nylon (PA)A–
Fluoropolymers
PTFEAA
FEPAA
PVDFAA
ECTFE/ETFEAA
Elastomers
EPDMA–
Viton (FPM)AA
NBRA–
Metals
SS 316AA
SS 304AA
AluminiumAA

Not rated in the source, so not in the table: PVC Rigid, PVC Flexible, PMP, Polystyrene, SAN, Polysulfone, Silicone

Resistance table: Sodium Nitrate, saturated

Material20 °C50 °CRemark
Thermoplastics
HDPEAA
LDPEAA
PPAA
PVC RigidAC
PVC FlexibleAC
PMPA–
PolystyreneAA
SANAA
PolycarbonateA–
PETGA*–
Acetal (POM)AA
Nylon (PA)A–
PolysulfoneA–
Fluoropolymers
PTFEAA
FEPAA
PVDFAA
ECTFE/ETFEAA
Elastomers
EPDMA–
Viton (FPM)AA
NBRBC
Metals
SS 316AA
SS 304AA
AluminiumAA

* estimated rating, given in the source without a temperature

Not rated in the source, so not in the table: Silicone

Rating scale

A rating marked * is an estimate in the source, not a test result. An estimate is given as one value without a temperature.

Frequently Asked Questions

Which materials resist Sodium Nitrate at high concentrations?

The materials with an A rating (resistant) for Sodium Nitrate at 20 °C are: PTFE, HDPE, PP, PVDF, PVC Rigid, EPDM, Viton (FPM), SS 316. These can generally be used in direct contact.

Does temperature affect chemical resistance to Sodium Nitrate?

Yes. 3 of 17 tested materials show a worse rating at 50 °C than at 20 °C for Sodium Nitrate. Materials affected include: PVC Rigid, NBR, PVC Flexible.

Is PTFE safe for Sodium Nitrate?

PTFE is rated A for Sodium Nitrate at 20 °C. A rating of A means resistant, B means limited resistance, C means partly resistant, and D means not resistant.

Does concentration affect chemical resistance to Sodium Nitrate?

Yes. Sodium Nitrate is tested at 2 concentrations (aqueous, saturated). Some materials change their rating depending on the concentration.

About this data

The ratings come from the chemical resistance list published by Bürkle GmbH, which compiled them from raw-material manufacturers’ data. They describe laboratory tests on the raw material at 20 °C and 50 °C.

A finished part also sees pressure, mechanical stress, welds and mixtures that a laboratory test does not. Treat the rating as a first filter and test under your own conditions before relying on it.

Chemicals with a similar resistance profile

Same 20 °C rating on the share of materials shown.